Bubbles of Ethylene Vinyl Acetate EVA Film Laminated Glass
By Peter Shin www.helloglass.com
Reason 1:
The plainness of the glass is not good. If you making tempered laminated glass, make sure the thickness of Ethylene Vinyl Acetate EVA film is thick enough.
Reason 2:
The Ethylene Vinyl Acetate EVA film is not melt completely when processing in the laminating vacuum oven, you need to increase the temperature or prolong the heating time to make sure Ethylene Vinyl Acetate EVA Film is melt completely.
Reason 3:
Stop vacuuming too early. Make sure you keep vacuuming always working in whole procedure of making laminated glass, and only stop the vacuuming after the temperature is lower than 45 degree C.
Reason 4:
The silicone bag is leaking, so the vacuuming pressure can not reach 0.095MPA.
Reason 5:
Moisture in the surface of glass, Ethylene Vinyl Acetate EVA Film, decorative interlayers is too much, please dry them before laminating.
Reason 6:
Part of laminated glass is suffering too high temperature, and lead to the Ethylene Vinyl Acetate EVA Film decompose to gas. Make sure the heating is well-distributed. And make sure the temperature detector is working well and get the correct temperature.
Reason 7:
When edging laminated glass, bubbles appear at the edges. Because edging makes heat, and too much heat causes the bubbles. Please use more water to cool laminated glass when edging, and edging slowly and softly if necessary.
Any other situation, please feel free to contact us.
ALL RIGHT RESERVED BY CNC INTERLAYER TECH :
(Product 1. )Ethylene-Vinyl Acetate Ethylene Vinyl Acetate Ethylene Vinyl Acetate EVAInterlayer Film for Safety Laminated Glass
(Product 2.) China Solar Ethylene Vinyl Acetate Ethylene Vinyl Acetate EVAFilm for Solar Panel Encapsulation
(Product 3.) China Smart Switchable Film for Privacy Glass, Smart Glass
(4)Web:www.Ethylene Vinyl Acetate EVAfilms.com / www.cncnext.com
(5)Contact Us: cnc@cncnext.com/ benext77@hotmail.com /benext77@gmail.com